Wednesday, October 29, 2008

Hamada Rust (Temmoku)


Hamada Rust cone 10

77.0 Custer Feldspar
0.1 Silica
6.2 Whiting
4.3 Kaolin
12.4 Gerstley Borate
7.5 Red Iron Oxide

Procelain, thrown and altered, cone 10 reduction.


John Britt
www.johnbrittpottery.com/wks.htm
www.penlandpottery.com/
http://ncclayclub.blogspot.com/

5 comments:

The Baby's Daddy said...

Dsmn, that's gorgeous. It's just missing a fly decal.

Eric Preece said...

Beautiful!

Carolanne said...

Very nice! Breaks beautifully. Did you by any chance note the SG when you mixed it up? 150? 160?

John Britt said...

Think it was sp. gr. 154

Carolanne said...

Excellent! Thanks.